Plans | Login    

Briefing Search
Keyword:
Category:

       

    
Author Details

Hot-rolled steel tube folding cause Analysis


Within the fold is a major quality defects in seamless pipe production is produced in the perforation process and can not be eliminated.

BriefingWire.com, 5/23/2014 - Within the fold is a fold on the inner surface of steel pipe, characterized by the appearance of scaly layer, similar to the closed curve, while there are irregular folds. Fold in the metal rolling process due to poor quality resulting from, when there is excessive segregation of non-metallic inclusions, there will be holes in the metal inclusions concentrated around the crack in the hole formed in the process of folding, after setting diameter after extrusion machine it scaly or other shapes appear. In short, the quality of rolled steel round billet failure is mainly non-metallic inclusions and harmful substances caused by the high degree of metal contamination. Moreover, when zonal segregation in the casting billet billet quality is extremely important for the impact. The zonal segregation depends largely on the steel chemical composition, thermal state and cooling rate. Steel increased levels of harmful elements to promote their segregation with concentration increase, thus the formation of segregation. In addition, the increase in carbon content will increase the segregation of impurities, especially manganese.

In the process of perforation following factors are also affected internal fold. Perforated internal fold of deformation parameters, but also with perforated steel folding process have a certain relationship between the perforation process parameter settings, tools, design for generating folded with some impact, not only the rupture of the tube center and roll the total pressure in the head before the total amount and the amount of pressure, but also to turn a half weeks with the tube of the amount of the partial pressure. perforated fold internal temperature effect: as the temperature increased, the plastic material to improve the critical pressure increase with temperature increases, but if it is using the best casting temperature casting tube, perforated at a certain temperature changes within the fold is no significant change in the. The heating time and within the fold of the relationship, when a certain temperature in the baked internal fold prolonged heating has little effect, but the number has increased significantly outside the fold, because the longer the heating time more severe grain growth, but the surface is more Obviously, the organization produced worse performance outside the fold. The tool off the impact of internal, internal off the head also have some impact, for example, head can reduce the use of nasal cavity to form their own holes, to improve the quality of the inner surface, while the shape of the head also have some impact on the quality, conical head will the tip from the head to pass part of the rolling reduction increases, which have an adverse impact on waste management; spherical head is able to ensure that waste management to reduce the amount of pressure along the feed direction, to improve the quality of waste management. The best head shape should be able to ensure that the deformation zone along the length of the same amount of pressure waste pipe wall thickness.

 
 
FAQs | Contact Us | Terms & Conditions | Privacy Policy
© 2026 Proserve Technology, Inc.